Select Language:
< Back LIMBALI (Gilbertiodendron brachystegioides) Print Friendly View
Limbali
Gilbertiodendron brachystegioides J.Leon.
LEGUMINOSAE
Abeum (Gabon); Ekoussek (Cameroon); Limbali
Macrolobium brachystegioides Harms
The tree is slightly buttressed. The bole is straight and cylindrical, may be up to 20 m in length, with diameters of 80 cm.
West Africa, Cameroon and Gabon.
Wood diffuse porous. Occasionally vessels exclusively solitary (over 90%). Tangential diameter of vessel lumina 200 micras or more (large). Vestured pits. Vessels per mm2 less than 6 (rare). Simple perforation plates. Vessel-ray pits similar to intervessel pits Occasionally axial parenchyma in marginal or in seemingly marginal bands. Axial parenchyma lozenge-aliform. Axial parenchyma aliform. Prismatic crystals in chambered axial parenchyma cells and/or in fibers. 3 to 4 cells per parenchyma strand. Rays more than 10 per mm (abundant). Occasionally rays and/or axial elements irregularly storied. Rays exclusively uniseriate. Body ray cells procumbent with mostly 2 to 4 rows of upright and/or square marginal cells (Kribs-II). Non-septate fibers. Fibers with simple to minutely bordered pits.
Unrestricted
The sapwood is white (outside) to brown (inside). The heartwood is brown with pale brown rings, it is clearly demarcated.
4
Straight or slightly interlocked, sometimes with an influence on further processing operations.
The texture of the wood is frequently coarse.
Luster is usually low.
Moderately durable to decay. Without preservative treatment, this species can be used only under risk of occasional re-humidification. It is not suited for uses with risks of permanent or long-lasting humidification. Moderately resistant to termites attack
3
No residual stresses are reported in this species.
Difficult to treat with only a low penetration of the preservative products.
0.64
0.71
9.2
4.5
Ease of Drying: It is reported to have a slow drying rate. Drying Defects: Risk of surface checks.
FR-6
2.0
1111
173600
611
81
78
626
720
It is moderately easy to saw.
Not suitable for slicing.
Not suitable for slicing.
Moderate blunting effect; stellited blades for sawing and carbide tools for machining are advised.
Possible difficulties caused by interlocked grain are reported.
Moderately easy; tools must be cautiously sharpened.
Moderately easy; tools must be cautiously sharpened.
30
Moderately easy; tools must be cautiously sharpened.
Moderately easy; tools must be cautiously sharpened.
Pre-boring is necessary.
Glues well if basic gluing technical rules are followed.
Easy to perform; it gives good results.
Needs pre-coating.
Working with hand tools is difficult.
EXTERIOR GENERAL, rails, HOUSING GENERAL, beams, joists, boards, flooring, parquet, frames, steps, panelling, fittings, TURNING, CONTAINERS, truck bodies, truck flooring, NAVAL CONSTRUCTION, boat deck, port storage